A twin-screw extrusion study found that curcumin, beetroot and chlorophyllin can be compounded into both polymers with modest effects on flow and mechanical properties, while spirulina fails in PLA and most formulations fade under xenon exposure.

Mirela ConstantinNovember 2, 20265 min read3 views

Four colored biopolymer masterbatch strands and injection-molded specimens on a laboratory bench, with extrusion equipment blurred behind them.

A study of natural pigments in polylactic acid (PLA) and polybutylene succinate (PBS) has found that several colorants can be incorporated into the biodegradable polymers using conventional melt processing, but thermal sensitivity and lightfastness still limit their use. The work focused on four commercial natural pigments: blue spirulina, yellow curcumin, red beetroot and green chlorophyllin.

The researchers produced color masterbatches by twin-screw extrusion and diluted them into the matching polymer at 2, 4 and 6 wt%. Test specimens were then made by injection molding. The masterbatch formulation also contained titanium dioxide, calcium carbonate and stearic acid to provide UV protection, support dispersion and aid processing.

Thermal limits shape the process

Natural pigments are organic materials and can begin to degrade at lower temperatures than the polymers they color. Thermogravimetric analysis put the degradation onset at about 229 °C for spirulina, 244 °C for curcumin, 258 °C for chlorophyllin and 267 °C for beetroot. PLA and PBS degrade at considerably higher temperatures, giving formulators room to melt the polymer while limiting exposure of the pigment.

The extrusion profiles reached 145 °C for PBS and 190 °C for PLA. The twin-screw extruder ran at 65 rpm with a feed rate of 2 kg/h. Most pigment–polymer combinations could be processed in this window. Spirulina was the clear exception: during PLA processing it lost its characteristic blue color, so a blue PLA masterbatch could not be produced. PBS, processed at the lower temperature, retained enough pigment stability for successful compounding.

Flow and mechanical effects are modest

From a processing standpoint, the pigments caused only limited changes in rheology. Melt flow rate fell slightly after incorporation, indicating a modest rise in melt viscosity. Neat PLA had an MFR of about 50 g/10 min, and the natural-pigment masterbatches stayed close to that value. PBS showed a similar response. The results suggest that most formulations would not require major changes to screw design, pressure settings or molding conditions.

Tensile and impact behavior also remained broadly stable across the 2–6 wt% range. PLA began with a Young’s modulus of about 1710 MPa and a tensile strength of 65.6 MPa; PBS began at about 392 MPa and 34.5 MPa. The colored formulations stayed close to those baselines. Impact strength remained in a similar range, although individual pigments produced some variation.

Light exposure is the main barrier

Successful extrusion did not guarantee durable color. After 50 hours of xenon-lamp exposure, most formulations showed a color difference above ΔE* = 2, indicating a visually perceptible change. The main exception was a PLA formulation containing 2 wt% green chlorophyllin masterbatch, which showed the highest photostability.

The study points to UV stability as the largest obstacle to broader use. Packaging, consumer products, agricultural parts and outdoor applications may need additional stabilization, protective coatings or pigment modification before natural colors can match conventional systems over long service periods.

The environmental comparison favored the natural pigments under the study’s assumptions. One kilogram of curcumin pigment generated about 0.04 kg CO2-eq, compared with 18.65 kg CO2-eq for the inorganic green reference pigment. The natural-pigment masterbatches also used less electricity during extrusion and pelletizing.

The study concludes that several natural colorants can be compounded into PLA and PBS with conventional equipment and with limited changes in melt viscosity and mechanical performance. Further work is still needed on lightfastness and thermal stability, particularly to preserve color during processing and subsequent service exposure.